Installation & Sealing Tips for Exchange Tundish Nozzle Assembly

Oct 22, 2026

The exchange tundish nozzle set is a key refractory part for continuous casting. It controls molten steel flow and casting speed. Bad installation or poor seal often causes steel leak, air suction, nozzle crack and casting stop. Below are simple, practical on-site tips for installation and sealing.

Check and clean before installation

  1. Check all parts: upper nozzle, zirconia core, lower nozzle, seat brick and sealing gasket. Do not use pieces with crack, chip or wrong size. Pay extra attention to the sealing face. Scratches on the contact surface will cause leak later.
  2. Clean the tundish bottom base completely. Clear steel slag, old mud and loose powder. Even small dirt will leave gaps and let steel run through or suck air when hot.
  3. Check the fitting gap. Normally keep the gap between nozzle and seat brick at 0.3–0.5 mm. Never hit hard with hammer when fitting. Hidden cracks will form and break during casting.
  4. Confirm nozzle inner size matches your steel grade and casting speed. Wrong bore size makes liquid level unstable and brings slag inclusion.

Installation steps

  1. Put the nozzle set straight along the steel flow channel. Keep it centered. Center offset should not exceed 2 mm. If off-center, molten steel hits one side, wears the nozzle fast and shortens service life.
  2. Put ceramic fiber gasket or high temp sealing mud on the joint evenly. For gasket, lay it flat, do not fold or tear. If using sealing mud, apply a thin layer. Too much mud will squeeze into the bore and block steel flow.
  3. Tighten the clamping device evenly from both sides. Do not tighten one side hard first. Uneven pressure will open the gap when parts expand under heat. For most sliding quick-change units, hydraulic pressure stays between 18–22 bar, follow maker's data.
  4. After locking, slide or swing the change mechanism two times by hand. It should move smoothly with no stuck. Stuck means misalignment or dirt between contact faces.

Key points for sealing

  1. Seal work has two targets: stop steel leak and stop cold air from getting in and re-oxidizing molten steel.
  2. Pick sealing material by your working condition. Ceramic fiber gasket works better if you change nozzles often. Sealing mud suits assemblies that rarely get replaced. Intumescent compound can be used as extra fill; it swells when heated to seal small gaps from different thermal expansion.
  3. For clean steel and low carbon steel, use argon shield around the joint. Keep low steady argon pressure. The gas barrier stops air suction and reduces alumina buildup inside nozzle.
  4. Do not mix different sealing materials. Do not stack mud with broken fiber scraps. Mixed filler has holes and fails easily under steel pressure.
  5. A tight seal at room temperature does not guarantee a good seal at high temperature. All joints must stay pressed tight after reaching tundish working temperature.

Baking rule after installation

Do not start casting right after installation. Heat up step by step. Fast heating causes thermal shock and cracks zirconia core and sealing layer. Standard baking: hold at 200–300 ℃ to remove water, then heat slowly to 900–1100 ℃ and keep soaking. Check joints after baking. Watch for smoke, air leak or hot spot before pouring. If leak sign shows, stop and redo the seal.

Watch during casting and hot exchange

  1. Check steel stream shape, mold level and joint temperature while casting. Twisted or shaking steel flow usually means off-center installation or broken seal.
  2. When you hot change lower nozzle on line, reduce air exposure time. Preheat spare nozzle set ahead. Cold spare part cracks immediately once touching hot molten steel.
  3. If steel seeps or air blows out from joint, stop casting following site rules. Do not burn the gap with oxygen lance while running.

Common mistakes to avoid

  • Reuse old deformed gaskets or skip cleaning
  • Put too much sealing mud into flow bore
  • Over-tighten and crush refractory contact surface
  • Ignore centering control
  • Skip staged baking and cast directly

 

 

For exchange tundish nozzle assembly, installation accuracy and sealing quality decide casting safety and sequence stability. Clean contact face, keep centered, choose proper sealing material, press evenly and bake step by step. These simple operations help reduce steel leak, air suction and early nozzle damage. Steel mills can cut refractory cost, lower unplanned stop and improve steel quality if operators follow these rules.