How to Judge the Right Timing to Exchange Tundish Nozzle On‑site?

Sep 23, 2026

Exchange tundish nozzle enables online replacement without terminating the whole tundish sequence, which greatly improves continuous casting productivity. However, many steel‑plant operators face practical confusion: when exactly should we perform on‑site nozzle exchange? Too‑early replacement increases refractory consumption cost; delayed exchange brings steel leakage risk, nozzle clogging and mass slab defects.

Anyang Changtai Silicon Industry Co., Ltd, as a professional manufacturer of zirconia‑based exchange tundish nozzle, summarizes practical on‑site judging standards accumulated from hundreds of steel‑mill service cases. Operators can make comprehensive judgment from visual inspection, dimensional measurement, molten‑steel stream performance, actual casting load and abnormal failure signals.

 

Visual On‑site Observation Signals

Visual check is the most direct method during casting operation. Operators should watch nozzle outer condition and steel stream status regularly.

Visible cracks, spalling or chipping on nozzle outer shell and working layer: thermal shock damage will expand rapidly under high temperature, trigger steel penetration hazard, immediate exchange required.

Obvious local erosion pit on nozzle outlet bore. Even if inner diameter is still within theoretical range, uneven erosion will distort steel flow pattern.

Molten‑steel stream swinging, diverging or splashing when exiting nozzle: stable cylindrical stream turns turbulent, which is typical warning for worn nozzle inner bore.

Tiny steel seepage or red‑hot trace around nozzle assembly: hidden risk of molten‑steel breakout, stop production and replace nozzle as soon as possible.

 

Dimensional Inspection: Inner‑Diameter Expansion Threshold

Zirconia insert suffers persistent scouring by high‑speed molten steel. Inner bore gradually enlarges during service. According to Changtai's application specification, exchange shall be arranged when inner‑diameter expansion exceeds 15% of original design size. For instance, if original bore is 50 mm, replacement is required once inner diameter reaches 57.5 mm or above.

Even expansion is below 15%, perform online exchange when detecting oval deformation, partial bulging or asymmetric wear. Deformed bore cannot maintain stable flow control, and will induce mould‑level fluctuation and slab slag inclusion. Dimensional measurement shall be completed during tundish turnaround or safe casting interval with dedicated measuring tools.

 

Molten‑Steel Flow & Casting‑Parameter Abnormalities

Production parameters reflect nozzle internal wear status which cannot be seen by naked eyes. These abnormal signals indicate approaching exchange timing:

Cannot maintain target casting speed even adjusting stopper or sliding gate to maximum opening; partial alumina clogging occurs inside nozzle bore. Argon purging cannot restore normal flow rate.

Frequent mould‑level violent fluctuation without ladle‑weight or tundish‑level disturbance. The unstable steel stream caused by worn nozzle disturbs mould flow field.

Gradually rising slab rejection rate for surface and internal inclusion defects under unchanged steel grade and casting process.

When above phenomena repeatedly occur, do not continue production for cost‑saving purpose; arrange on‑line exchange of tundish nozzle in next safe window.

 

Actual Casting Load & Designed Service‑Life Reference

Every exchange tundish nozzle from Changtai has recommended service scope based on material formula. Standard CNM exchange nozzle normally supports 10‑15 heats under regular carbon‑steel casting condition.

Operators need to record real steel throughput and accumulated casting time for each nozzle. Do not rigidly follow fixed furnace number:

For high‑aluminum killed steel, high‑Mn alloy steel, casting speed uplift or over‑heating molten steel, erosion rate accelerates, exchange cycle should be shortened properly.

For low‑carbon plain steel under moderate casting speed, service life can approach upper design limit with stable working condition.

Design service life acts as reference baseline, not absolute threshold. Combine visual, dimensional and parameter status to make final decision.

 

Emergency Forced‑exchange Conditions

Under following emergency situations, execute immediate nozzle exchange regardless of remaining theoretical service life:

Nozzle body cracks or refractory peeling‑off observed;

Partial perforation risk and steel seepage symptom;

Severe clogging which cannot be eliminated, continuous casting speed drops sharply;

Large‑area spalling of zirconia working layer, refractory fragments dropping into molten steel.

 

Online quick‑change mechanism is designed to maximize tundish sequence length, but cannot be used for unlimited service extension. Establish standardized nozzle inspection log, identify warning signals in advance and complete timely exchange, so as to balance refractory cost, casting safety and finished‑slab quality.

If you need technical support for exchange tundish nozzle selection, custom formulation or on‑site application guidance, please feel free to contact Changtai's engineering team.